Characteristics for grade     MNMts43-0.5   ( МНМц43-0.5 )



      Grade :   MNMts43-0.5   ( МНМц43-0.5 ) (   Копель   )
      Classification :   Copper-nickel alloys
      Equivalent grades:   Go here



Chemical composition in % for grade   MNMts43-0.5   ( МНМц43-0.5 )
Ni+Co Fe C Si Mn S P Cu As Pb Mg Sb Bi Impurity
42.5 - 44max   0.15max   0.1max   0.10.1 - 1max   0.01max   0.00254.4 - 57.4max   0.002max   0.002max   0.05max   0.002max   0.002 all 0.6
Comment: Cu is a basis; the percentage of Cu is given approximately.


Mechanical properties under Т=20oС for grade   MNMts43-0.5   ( МНМц43-0.5 )
Assortment Dimension Direct. sв sT d5 y KCU Heat treatment
- mm - MPa MPa % % kJ / m2 -
Wire, GOST 22666-77 Ø 0.2 - 0.5   390   15-20   
soft     380-460  35-42   
hard     600-700  3-4   


    Brinell hardness for     MNMts43-0.5   ( МНМц43-0.5 )   ,     soft HB 10 -1 = 85 - 90   MPa
    Brinell hardness for     MNMts43-0.5   ( МНМц43-0.5 )   ,     hard HB 10 -1 = 185   MPa


Technological properties of the material   MNMts43-0.5   ( МНМц43-0.5 ) .
        Melting temperature : 1290   °C
        Forging temperature : 1000 - 1150   °C
        Annealing temperature : 800 - 850   °C


Physical properties for grade   MNMts43-0.5   ( МНМц43-0.5 )
T E 10- 5 a 10 6 l r C R 10 9
Grade MPa 1/Grade Watt/(m·Grade) kg/m3 J/(kg·Grade) Ohm·m
20 1.2   24.4 8900   490
100   14        


Equivalent steels for grade     MNMts43-0.5   ( МНМц43-0.5 )
Warning! Indicated both exact and nearest equivalents.
GermanyFranceItalyPolandCzechiaAustriaInter
DIN,WNrAFNORUNIPNCSNONORMISO
CuNi44Mn1
CuNi44Mn
PCuNi44Mn1
CuNi44Mn1
423065
CuNi44Mn1
CuNi44Mn1



Types of delivery of grade   MNMts43-0.5   ( МНМц43-0.5 )
B51 - Non-ferrous metals, including rare metals, and their alloys
B74 - Wire made of non-ferrous metals and their alloys


Specification :
Mechanical properties :
sв - Tensile strength , [MPa]
sT - Yield stress, [MPa]
d5 - Specific elongation at fracture , [ % ]
y - Reduction of area , [ % ]
KCU - Impact strength , [ kJ / m2]
HB - Brinell hardness , [MPa]

Physical properties :
T - Test temperature , [Grade]
E - Young modulus , [MPa]
a - Coefficient of linear expansion (range 20o - T ) , [1/Grade]
l - Termal (heat) condition coefficient , [Watt/(m·Grade)]
r - Density , [kg/m3]
C - Specific heat ( range 20o - T ), [J/(kg·Grade)]
R - Electrical resistance , [Ohm·m]

  MNMts43-0.5   ( МНМц43-0.5 ) - Copper-nickel alloys: chemical composition, mechanical and physical properties, hardness
Database of steels and alloys (Marochnik) contains information about chemical composition and properties more then 3000 steels and alloys