Database of Steel and Alloy (Marochnik)

  Home     Steel and Alloy     Search     Equivalent Grades     GOST Standards     Grading     Contacts  
   
YOU HERE:   Steel and Alloy   ->   Structural steel

Characteristics for grade     18G2АFps   ( 18Г2АФпс )

      Grade :     18G2АFps   ( 18Г2АФпс )
      Substitute:   16Г2АФ, 10ХСНД, 15ХСНД
      Classification :   Structural steel for welding construct
      Equivalent grades:   Go here



Chemical composition in % for grade   18G2АFps   ( 18Г2АФпс )
C Si Mn Ni S P Cr V N Cu As
0.14 - 0.22max   0.171.3 - 1.7max   0.3max   0.04max   0.035max   0.30.08 - 0.150.015 - 0.03max   0.3max   0.08


Temperature of critical points for grade   18G2АFps   ( 18Г2АФпс ).
Ac1 = 720 ,      Ac3(Acm) = 880 ,       Ar3(Arcm) = 780 ,       Ar1 = 620


Mechanical properties under Т=20oС for grade   18G2АFps   ( 18Г2АФпс )
Assortment Dimension Direct. sв sT d5 y KCU Heat treatment
- mm - MPa MPa % % kJ / m2 -
Sheet, GOST 19282-73     590 440 19    


Technological properties for grade   18G2АFps   ( 18Г2АФпс )
  Weldability: without limitations.


Equivalent steels for grade     18G2АFps   ( 18Г2АФпс )
Warning! Indicated both exact and nearest equivalents.
USAGermanyJapanFranceEnglandEuropeanItalySpainChinaSwedenHungaryPolandSwitzerland
-DIN,WNrJIS AFNORBSEN UNIUNEGBSSMSZPNSNV
A633Gr.E
K02900
K12202
1.8905
P355N
P460N
StE355
StE460
SM520B
SM520C
E460RIFP
FeE460KGN
P460N
4360-55F
55F
P460N
1.8901
1.8905
FeE460KG
FeE460KW
P460N
S460N
FeE460KG
P460N
AE460KG
P460N
15MnVNR
18MnMoNbR
Q460C
2143
E460D
18G2AV
StE47

Types of delivery of grade   18G2АFps   ( 18Г2АФпс )
В22 - Graded and shaped rolling
B33 - Sheets and Strips
В62 - Steel pipes and connecting parts to them


Specification :
Mechanical properties :
sв - Tensile strength , [MPa]
sT - Yield stress, [MPa]
d5 - Specific elongation at fracture , [ % ]
y - Reduction of area , [ % ]
KCU - Impact strength , [ kJ / m2]
HB - Brinell hardness , [MPa]

Physical properties :
T - Test temperature , [Grade]
E - Young modulus , [MPa]
a - Coefficient of linear expansion (range 20o - T ) , [1/Grade]
l - Termal (heat) condition coefficient , [Watt/(m·Grade)]
r - Density , [kg/m3]
C - Specific heat ( range 20o - T ), [J/(kg·Grade)]
R - Electrical resistance , [Ohm·m]

Weldability :
without limitations - welding is done without heating and subsequent heat treeting
limited weldability - welding is possible under heating up to 100-120 grade and subsequent heat treeting
hard weldability - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing

  18G2АFps   ( 18Г2АФпс ) - Structural steel for welding construct: chemical composition, mechanical and physical properties, hardness
Database of steels and alloys (Marochnik) contains information about chemical composition and properties more then 3000 steels and alloys

    ©   2003 - 2019         Database of Steel and Alloy (russian title is the Marochnik)
Administration of the Marochnik is not responsible for the content's use.