Database of Steel and Alloy (Marochnik) |
Home | Steel and Alloy | Search | Equivalent Grades | GOST Standards | Grading | Contacts |
Grade : | 10KHSND ( 10ХСНД ) ( 10ХСНД-Ш ) |
Substitute: | 16Г2АФ |
Classification : | Structural steel for welding construct |
Equivalent grades: | Go here |
C | Si | Mn | Ni | S | P | Cr | V | N | Cu | As |
max 0.12 | 0.8 - 1.1 | 0.5 - 0.8 | 0.5 - 0.8 | max 0.035 | max 0.03 | 0.6 - 0.9 | max 0.12 | max 0.008 | 0.4 - 0.6 | max 0.08 |
Assortment | Dimension | Direct. | sв | sT | d5 | y | KCU | Heat treatment |
- | mm | - | MPa | MPa | % | % | kJ / m2 | - |
Sheet, GOST 19282-73 | 5 - 9 | 540 | 400 | 19 | ||||
Rolled stock, GOST 6713-91 | 510-685 | 390 | 19 | 290 | ||||
Bars | to 50 | 530 | 390 | 18 |
Weldability: | without limitations. |
Flakes : | not predisposed |
Temper brittleness: | weakly predisposed |
T | E 10- 5 | a 10 6 | l | r | C | R 10 9 |
Grade | MPa | 1/Grade | Watt/(m·Grade) | kg/m3 | J/(kg·Grade) | Ohm·m |
20 | ||||||
100 | 1.97 | 40 | ||||
200 | 2.01 | 39 | ||||
300 | 1.95 | 38 | ||||
400 | 1.88 | 36 | ||||
500 | 1.8 | 34 | ||||
600 | 1.69 | 31 | ||||
700 | 1.56 | 29 | ||||
800 | 1.35 | |||||
900 | 1.25 | |||||
T | E 10- 5 | a 10 6 | l | r | C | R 10 9 |
Bulgaria | |
BDS | |
|
В22 - Graded and shaped rolling |
B23 - Sheets and Strips |
B33 - Sheets and Strips |
В62 - Steel pipes and connecting parts to them |
Mechanical properties : | |
sв | - Tensile strength , [MPa] |
sT | - Yield stress, [MPa] |
d5 | - Specific elongation at fracture , [ % ] |
y | - Reduction of area , [ % ] |
KCU | - Impact strength , [ kJ / m2] |
HB | - Brinell hardness , [MPa] |
Physical properties : | |
T | - Test temperature , [Grade] |
E | - Young modulus , [MPa] |
a | - Coefficient of linear expansion (range 20o - T ) , [1/Grade] |
l | - Termal (heat) condition coefficient , [Watt/(m·Grade)] |
r | - Density , [kg/m3] |
C | - Specific heat ( range 20o - T ), [J/(kg·Grade)] |
R | - Electrical resistance , [Ohm·m] |
Weldability : | |
without limitations | - welding is done without heating and subsequent heat treeting |
limited weldability | - welding is possible under heating up to 100-120 grade and subsequent heat treeting |
hard weldability | - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing |