Grade : | U7 ( У7 ) |
Substitute: | У8 |
Classification : | Carbon tool steel |
Equivalent grades: | Go here |
C | Si | Mn | Ni | S | P | Cr | Cu |
0.65 - 0.74 | 0.17 - 0.33 | 0.17 - 0.33 | max 0.25 | max 0.028 | max 0.03 | max 0.2 | max 0.25 |
Ac1 = 730 , Ac3(Acm) = 770 , Ar1 = 700 , Mn = 280 |
Assortment | Dimension | Direct. | sв | sT | d5 | y | KCU | Heat treatment |
- | mm | - | MPa | MPa | % | % | kJ / m2 | - |
Band cold-rolled | to 1 | 650 | 15 | As-delivered state |
Brinell hardness for U7 ( У7 ) (annealing) , GOST 1435-99 | HB 10 -1 = 187 MPa |
Weldability: | is not used. |
Flakes : | not predisposed |
Temper brittleness: | not predisposed |
T | E 10- 5 | a 10 6 | l | r | C | R 10 9 |
Grade | MPa | 1/Grade | Watt/(m·Grade) | kg/m3 | J/(kg·Grade) | Ohm·m |
20 | 46 | 7830 | 130 | |||
100 | 46 | |||||
200 | ||||||
300 | 41 | 580 | ||||
400 | 664 | |||||
500 | 819 | |||||
600 | 33 | 970 | ||||
700 | 710 | |||||
800 | 706 | |||||
900 | 29 | 685 | ||||
T | E 10- 5 | a 10 6 | l | r | C | R 10 9 |
Germany | Japan | France | European | Italy | China | Bulgaria | Hungary | Poland | Romania | Czechia | Austria | ||||||||||||||||||||
DIN,WNr | JIS | AFNOR | EN | UNI | GB | BDS | MSZ | PN | STAS | CSN | ONORM | ||||||||||||||||||||
|
|
|
|
|
|
|
|
|
|
|
|
В22 - Graded and shaped rolling |
B23 - Sheets and Strips |
В32 - Graded and shaped rolling |
B33 - Sheets and Strips |
B34 - Ribbons |
В72 - Medium-high and high-carbon steel wire |
Mechanical properties : | |
sв | - Tensile strength , [MPa] |
sT | - Yield stress, [MPa] |
d5 | - Specific elongation at fracture , [ % ] |
y | - Reduction of area , [ % ] |
KCU | - Impact strength , [ kJ / m2] |
HB | - Brinell hardness , [MPa] |
Physical properties : | |
T | - Test temperature , [Grade] |
E | - Young modulus , [MPa] |
a | - Coefficient of linear expansion (range 20o - T ) , [1/Grade] |
l | - Termal (heat) condition coefficient , [Watt/(m·Grade)] |
r | - Density , [kg/m3] |
C | - Specific heat ( range 20o - T ), [J/(kg·Grade)] |
R | - Electrical resistance , [Ohm·m] |
Weldability : | |
without limitations | - welding is done without heating and subsequent heat treeting |
limited weldability | - welding is possible under heating up to 100-120 grade and subsequent heat treeting |
hard weldability | - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing |
© 2003 - 2025 Database of Steel and Alloy (russian title is the Marochnik)