Characteristics for grade     АL8   ( АЛ8 )



      Grade :     АL8   ( АЛ8 )
      Classification :   Aluminium casting alloys
      Equivalent grades:   Go here



Chemical composition in % for grade   АL8   ( АЛ8 )
Fe Si Mn TiAl Cu Zr Be Mg Zn Impurity
max   0.3max   0.3max   0.1max   0.0789 - 90.5max   0.1max   0.2max   0.079.5 - 10max   0.1 all 1
Comment: Al is a basis; the percentage of Al is given approximately.


Mechanical properties under Т=20oС for grade   АL8   ( АЛ8 )
Assortment Dimension Direct. sв sT d5 y KCU Heat treatment
- mm - MPa MPa % % kJ / m2 -
sand (mould) casting     320 170 11  1000 


    Brinell hardness for     АL8   ( АЛ8 )   ,     sand (mould) casting HB 10 -1 = 70   MPa


Technological properties of the material   АL8   ( АЛ8 ) .
        Linear shrinkage : 1.3   %


Physical properties for grade   АL8   ( АЛ8 )
T E 10- 5 a 10 6 l r C R 10 9
Grade MPa 1/Grade Watt/(m·Grade) kg/m3 J/(kg·Grade) Ohm·m
20 0.7     2550   91.2
100   24.5 96.4   1050  


Equivalent steels for grade     АL8   ( АЛ8 )
Warning! Indicated both exact and nearest equivalents.
USAGermanyJapanEnglandChinaInter
-DIN,WNrJIS BSGBISO
A05200
G-AlMg10
AC7B
LM10
ZAlMg10
ZL301
AlMg10




Specification :
Mechanical properties :
sв - Tensile strength , [MPa]
sT - Yield stress, [MPa]
d5 - Specific elongation at fracture , [ % ]
y - Reduction of area , [ % ]
KCU - Impact strength , [ kJ / m2]
HB - Brinell hardness , [MPa]

Physical properties :
T - Test temperature , [Grade]
E - Young modulus , [MPa]
a - Coefficient of linear expansion (range 20o - T ) , [1/Grade]
l - Termal (heat) condition coefficient , [Watt/(m·Grade)]
r - Density , [kg/m3]
C - Specific heat ( range 20o - T ), [J/(kg·Grade)]
R - Electrical resistance , [Ohm·m]

  АL8   ( АЛ8 ) - Aluminium casting alloys: chemical composition, mechanical and physical properties, hardness
Database of steels and alloys (Marochnik) contains information about chemical composition and properties more then 3000 steels and alloys

    ©   2003 - 2025         Database of Steel and Alloy (russian title is the Marochnik)
Administration of the Marochnik is not responsible for the content's use.
Рейтинг@Mail.ru