Grade : | 9KH1 ( 9Х1 ) |
Substitute: | 9Х2 |
Classification : | Alloy tool steel |
Equivalent grades: | Go here |
C | Si | Mn | Ni | S | P | Cr | Mo | W | V | Ti | Cu |
0.8 - 0.95 | 0.25 - 0.45 | 0.15 - 0.4 | max 0.4 | max 0.03 | max 0.03 | 1.4 - 1.7 | max 0.2 | max 0.2 | max 0.15 | max 0.03 | max 0.3 |
Ac1 = 745 , Ac3(Acm) = 860 , Ar1 = 700 , Mn = 270 |
Assortment | Dimension | Direct. | sв | sT | d5 | y | KCU | Heat treatment |
- | mm | - | MPa | MPa | % | % | kJ / m2 | - |
880 | 830 | 12 | 37 | 700 | Guenching Drawing 500oC, |
Brinell hardness for 9KH1 ( 9Х1 ) (annealing) , GOST 5950-2000 | HB 10 -1 = 229 MPa |
Weldability: | is not used. |
Flakes : | predisposed |
Temper brittleness: | weakly predisposed |
Germany | China | Czechia | Austria | |||||
DIN,WNr | GB | CSN | ONORM | |||||
|
|
|
|
В32 - Graded and shaped rolling |
Mechanical properties : | |
sв | - Tensile strength , [MPa] |
sT | - Yield stress, [MPa] |
d5 | - Specific elongation at fracture , [ % ] |
y | - Reduction of area , [ % ] |
KCU | - Impact strength , [ kJ / m2] |
HB | - Brinell hardness , [MPa] |
Physical properties : | |
T | - Test temperature , [Grade] |
E | - Young modulus , [MPa] |
a | - Coefficient of linear expansion (range 20o - T ) , [1/Grade] |
l | - Termal (heat) condition coefficient , [Watt/(m·Grade)] |
r | - Density , [kg/m3] |
C | - Specific heat ( range 20o - T ), [J/(kg·Grade)] |
R | - Electrical resistance , [Ohm·m] |
Weldability : | |
without limitations | - welding is done without heating and subsequent heat treeting |
limited weldability | - welding is possible under heating up to 100-120 grade and subsequent heat treeting |
hard weldability | - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing |