Grade : | 9KHS ( 9ХС ) |
Substitute: | ХВГ, ХВСГ |
Classification : | Alloy tool steel |
Equivalent grades: | Go here |
C | Si | Mn | Ni | S | P | Cr | Mo | W | V | Ti | Cu |
0.85 - 0.95 | 1.2 - 1.6 | 0.3 - 0.6 | max 0.4 | max 0.03 | max 0.03 | 0.95 - 1.25 | max 0.2 | max 0.2 | max 0.15 | max 0.03 | max 0.3 |
Ac1 = 770 , Ac3(Acm) = 870 , Ar1 = 730 , Mn = 160 |
Assortment | Dimension | Direct. | sв | sT | d5 | y | KCU | Heat treatment |
- | mm | - | MPa | MPa | % | % | kJ / m2 | - |
790 | 445 | 26 | 54 | 390 | As-delivered state |
Brinell hardness for 9KHS ( 9ХС ) (annealing) , GOST 5950-2000 | HB 10 -1 = 241 MPa |
Weldability: | is not used. |
Flakes : | not predisposed |
Temper brittleness: | predisposed |
T | E 10- 5 | a 10 6 | l | r | C | R 10 9 |
Grade | MPa | 1/Grade | Watt/(m·Grade) | kg/m3 | J/(kg·Grade) | Ohm·m |
20 | 1.9 | 7830 | 400 |
Germany | |||
DIN,WNr | |||
|
В32 - Graded and shaped rolling |
Mechanical properties : | |
sв | - Tensile strength , [MPa] |
sT | - Yield stress, [MPa] |
d5 | - Specific elongation at fracture , [ % ] |
y | - Reduction of area , [ % ] |
KCU | - Impact strength , [ kJ / m2] |
HB | - Brinell hardness , [MPa] |
Physical properties : | |
T | - Test temperature , [Grade] |
E | - Young modulus , [MPa] |
a | - Coefficient of linear expansion (range 20o - T ) , [1/Grade] |
l | - Termal (heat) condition coefficient , [Watt/(m·Grade)] |
r | - Density , [kg/m3] |
C | - Specific heat ( range 20o - T ), [J/(kg·Grade)] |
R | - Electrical resistance , [Ohm·m] |
Weldability : | |
without limitations | - welding is done without heating and subsequent heat treeting |
limited weldability | - welding is possible under heating up to 100-120 grade and subsequent heat treeting |
hard weldability | - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing |