Grade : | АV ( АВ ) ( 1340 ) |
Classification : | Aluminium wrought alloys |
Equivalent grades: | Go here |
Fe | Si | Mn | Cr | Ti | Al | Cu | Mg | Zn | Impurity |
max 0.5 | 0.5 - 1.2 | 0.15 - 0.35 | max 0.25 | max 0.15 | 95.95 - 98.8 | 0.1 - 0.5 | 0.45 - 0.9 | max 0.2 | other, each 0.05; all 0.1 |
Assortment | Dimension | Direct. | sв | sT | d5 | y | KCU | Heat treatment |
- | mm | - | MPa | MPa | % | % | kJ / m2 | - |
Pipe, GOST 18482-79 | 210 | 110 | 14 | Hardening and ageing | ||||
Pipe, GOST 18482-79 | 310 | 225 | 8 | Quenching and artificial aging | ||||
Bar, GOST 21488-97 | 175 | 100 | 14 | Hardening and ageing | ||||
Bar, GOST 21488-97 | 295 | 225 | 12 | Quenching and artificial aging | ||||
Bar, GOST 51834-2001 | 335 | 245 | 8 | Quenching and artificial aging | ||||
Bar, GOST 51834-2001 | 295-315 | 225 | 12-14 | Quenching and artificial aging | ||||
Band annealed , GOST 13726-97 | 145 | 15 | ||||||
Profile, GOST 8617-81 | to 50 | 294 | 225 | 10 | Quenching and artificial aging | |||
Profile, GOST 8617-81 | 176 | 14 | ||||||
Plate , GOST 17232-99 | 165-175 | 10-14 | Hardening and ageing | |||||
Plate , GOST 17232-99 | 275-295 | 6-7 | Quenching and artificial aging |
Brinell hardness for АV ( АВ ) , | HB 10 -1 = 85 MPa |
Brinell hardness for АV ( АВ ) (quenching) , | HB 10 -1 = 65 MPa |
Brinell hardness for АV ( АВ ) , annealed | HB 10 -1 = 30 MPa |
T | E 10- 5 | a 10 6 | l | r | C | R 10 9 |
Grade | MPa | 1/Grade | Watt/(m·Grade) | kg/m3 | J/(kg·Grade) | Ohm·m |
20 | 0.71 | 2700 | 37 | |||
100 | 23.5 | 180 | 797 |
USA | Japan | ||
- | JIS | ||
|
|
B52 - Graded and shaped rolling |
B53 - Sheets and Strips |
В54 - Ribbons |
B55 - Bars |
B64 - Pipes of non-ferrous metals and alloys |
Mechanical properties : | |
sв | - Tensile strength , [MPa] |
sT | - Yield stress, [MPa] |
d5 | - Specific elongation at fracture , [ % ] |
y | - Reduction of area , [ % ] |
KCU | - Impact strength , [ kJ / m2] |
HB | - Brinell hardness , [MPa] |
Physical properties : | |
T | - Test temperature , [Grade] |
E | - Young modulus , [MPa] |
a | - Coefficient of linear expansion (range 20o - T ) , [1/Grade] |
l | - Termal (heat) condition coefficient , [Watt/(m·Grade)] |
r | - Density , [kg/m3] |
C | - Specific heat ( range 20o - T ), [J/(kg·Grade)] |
R | - Electrical resistance , [Ohm·m] |