Characteristics for grade     12KH2N4А   ( 12Х2Н4А )

      Grade :     12KH2N4А   ( 12Х2Н4А )
      Substitute:   20ХГНР, 12ХН2, 12ХН3А, 20Х2Н4А, 20ХГР
      Classification :   Alloy structurall steel
      Equivalent grades:   Go here



Chemical composition in % for grade   12KH2N4А   ( 12Х2Н4А )
C Si Mn Ni S P Cr Cu
0.09 - 0.150.17 - 0.370.3 - 0.63.25 - 3.65max   0.025max   0.0251.25 - 1.65max   0.3


Temperature of critical points for grade   12KH2N4А   ( 12Х2Н4А ).
Ac1 = 745 ,      Ac3(Acm) = 800 ,       Ar3(Arcm) = 675 ,       Ar1 = 625 ,       Mn = 438


Mechanical properties under Т=20oС for grade   12KH2N4А   ( 12Х2Н4А )
Assortment Dimension Direct. sв sT d5 y KCU Heat treatment
- mm - MPa MPa % % kJ / m2 -
Bar, GOST 4543-71 Ø 15   1130 930 10 50880Guenching and drawing


    Brinell hardness for     12KH2N4А   ( 12Х2Н4А )   (annealing) ,       GOST 4543-71 HB 10 -1 = 269   MPa


Technological properties for grade   12KH2N4А   ( 12Х2Н4А )
  Weldability: limited weldability.
 Flakes : predisposed
Temper brittleness: predisposed


Physical properties for grade   12KH2N4А   ( 12Х2Н4А )
T E 10- 5 a 10 6 l r C R 10 9
Grade MPa 1/Grade Watt/(m·Grade) kg/m3 J/(kg·Grade) Ohm·m
20 2     7840    
100   11 25 7820    
200   12        
300   13   7760    
400   14.7 19 7710    
500   15.3        
600   15.6   7630    
T E 10- 5 a 10 6 l r C R 10 9


Equivalent steels for grade     12KH2N4А   ( 12Х2Н4А )
Warning! Indicated both exact and nearest equivalents.
USAGermanyJapanFranceEnglandBulgariaPolandCzechia
-DIN,WNrJIS AFNORBSBDSPNCSN
3310H
E3310
E3310X
G33106
1.5752
14NiCr14
X12Ni5
SNC815
13NiCr14
655H13
655M13
12Ch2N4A
12H2N4A
16420

Types of delivery of grade   12KH2N4А   ( 12Х2Н4А )
В22 - Graded and shaped rolling
B23 - Sheets and Strips
В32 - Graded and shaped rolling


Specification :
Mechanical properties :
sв - Tensile strength , [MPa]
sT - Yield stress, [MPa]
d5 - Specific elongation at fracture , [ % ]
y - Reduction of area , [ % ]
KCU - Impact strength , [ kJ / m2]
HB - Brinell hardness , [MPa]

Physical properties :
T - Test temperature , [Grade]
E - Young modulus , [MPa]
a - Coefficient of linear expansion (range 20o - T ) , [1/Grade]
l - Termal (heat) condition coefficient , [Watt/(m·Grade)]
r - Density , [kg/m3]
C - Specific heat ( range 20o - T ), [J/(kg·Grade)]
R - Electrical resistance , [Ohm·m]

Weldability :
without limitations - welding is done without heating and subsequent heat treeting
limited weldability - welding is possible under heating up to 100-120 grade and subsequent heat treeting
hard weldability - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing

  12KH2N4А   ( 12Х2Н4А ) - Alloy structurall steel: chemical composition, mechanical and physical properties, hardness
Database of steels and alloys (Marochnik) contains information about chemical composition and properties more then 3000 steels and alloys

    ©   2003 - 2019         Database of Steel and Alloy (russian title is the Marochnik)
Administration of the Marochnik is not responsible for the content's use.
Previous address of this website was splav.kharkov.com
Рейтинг@Mail.ru