Database of Steel and Alloy (Marochnik) |
Home | Steel and Alloy | Search | Equivalent Grades | GOST Standards | Grading | Contacts |
Grade : | 8KH3 ( 8Х3 ) |
Substitute: | 7Х3 |
Classification : | Die tool steel |
Equivalent grades: | Is absent |
C | Si | Mn | Ni | S | P | Cr | Mo | W | V | Ti | Cu |
0.75 - 0.85 | 0.1 - 0.4 | 0.15 - 0.45 | max 0.4 | max 0.03 | max 0.03 | 3.2 - 3.8 | max 0.2 | max 0.2 | max 0.15 | max 0.03 | max 0.3 |
Ac1 = 785 , Ac3(Acm) = 830 , Ar3(Arcm) = 770 , Ar1 = 750 , Mn = 370 |
Assortment | Dimension | Direct. | sв | sT | d5 | y | KCU | Heat treatment |
- | mm | - | MPa | MPa | % | % | kJ / m2 | - |
1340 | 1270 | 8 | 25 | 340 | Guenching 870oC, oil, Drawing 500oC, 2h, |
Brinell hardness for 8KH3 ( 8Х3 ) (annealing) , GOST 5950-2000 | HB 10 -1 = 241 MPa |
В22 - Graded and shaped rolling |
B31 - Blanks, Blanks, Slabs |
В32 - Graded and shaped rolling |
B33 - Sheets and Strips |
Mechanical properties : | |
sв | - Tensile strength , [MPa] |
sT | - Yield stress, [MPa] |
d5 | - Specific elongation at fracture , [ % ] |
y | - Reduction of area , [ % ] |
KCU | - Impact strength , [ kJ / m2] |
HB | - Brinell hardness , [MPa] |
Physical properties : | |
T | - Test temperature , [Grade] |
E | - Young modulus , [MPa] |
a | - Coefficient of linear expansion (range 20o - T ) , [1/Grade] |
l | - Termal (heat) condition coefficient , [Watt/(m·Grade)] |
r | - Density , [kg/m3] |
C | - Specific heat ( range 20o - T ), [J/(kg·Grade)] |
R | - Electrical resistance , [Ohm·m] |
© 2003 - 2025 Database of Steel and Alloy (russian title is the Marochnik)