Grade : | 4KH5MFS ( 4Х5МФС ) |
Substitute: | 4Х5МФ1С, 4Х4ВМФС |
Classification : | Die tool steel |
Equivalent grades: | Go here |
C | Si | Mn | Ni | S | P | Cr | Mo | V | Cu |
0.32 - 0.4 | 0.9 - 1.2 | 0.2 - 0.5 | max 0.4 | max 0.03 | max 0.03 | 4.5 - 5.5 | 1.2 - 1.5 | 0.3 - 0.5 | max 0.3 |
Ac1 = 840 , Ac3(Acm) = 870 , Ar3(Arcm) = 810 , Ar1 = 735 , Mn = 300 |
Assortment | Dimension | Direct. | sв | sT | d5 | y | KCU | Heat treatment |
- | mm | - | MPa | MPa | % | % | kJ / m2 | - |
Bars | 10 | 1750 | 1480 | 570 | Guenching 1000 - 1020oC,Drawing 530 - 560oC,Drawing 500 - 520oC, |
Brinell hardness for 4KH5MFS ( 4Х5МФС ) (annealing) , GOST 5950-2000 | HB 10 -1 = 241 MPa |
T | E 10- 5 | a 10 6 | l | r | C | R 10 9 |
Grade | MPa | 1/Grade | Watt/(m·Grade) | kg/m3 | J/(kg·Grade) | Ohm·m |
20 | 29 | 7750 | 480 | |||
100 | 30 | 7724 | ||||
200 | 30 | 7697 | ||||
300 | 31 | 7670 | ||||
400 | 33 | 7641 | ||||
500 | 31 | 7600 | ||||
600 | 30 | 7573 | ||||
700 | 28 | 7546 | ||||
800 | 26 | 7520 | ||||
900 | 27 | 7495 | ||||
T | E 10- 5 | a 10 6 | l | r | C | R 10 9 |
USA | Germany | Japan | France | England | European | Italy | Spain | China | Bulgaria | Poland | Romania | Czechia | Austria | South Korea | ||||||||||||||||||||||||||
- | DIN,WNr | JIS | AFNOR | BS | EN | UNI | UNE | GB | BDS | PN | STAS | CSN | ONORM | KS | ||||||||||||||||||||||||||
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
В22 - Graded and shaped rolling |
B31 - Blanks, Blanks, Slabs |
В32 - Graded and shaped rolling |
B33 - Sheets and Strips |
Mechanical properties : | |
sв | - Tensile strength , [MPa] |
sT | - Yield stress, [MPa] |
d5 | - Specific elongation at fracture , [ % ] |
y | - Reduction of area , [ % ] |
KCU | - Impact strength , [ kJ / m2] |
HB | - Brinell hardness , [MPa] |
Physical properties : | |
T | - Test temperature , [Grade] |
E | - Young modulus , [MPa] |
a | - Coefficient of linear expansion (range 20o - T ) , [1/Grade] |
l | - Termal (heat) condition coefficient , [Watt/(m·Grade)] |
r | - Density , [kg/m3] |
C | - Specific heat ( range 20o - T ), [J/(kg·Grade)] |