Database of Steel and Alloy (Marochnik) |
Home | Steel and Alloy | Search | Equivalent Grades | GOST Standards | Grading | Contacts |
Grade : | 9KH2MF ( 9Х2МФ ) |
Classification : | Tool steel for roller |
Equivalent grades: | Is absent |
C | Si | Mn | Ni | S | P | Cr | Mo | V |
0.85 - 0.95 | 0.25 - 0.5 | 0.2 - 0.7 | max 0.5 | max 0.03 | max 0.03 | 1.7 - 2.1 | 0.2 - 0.3 | 0.1 - 0.2 |
Ac1 = 748 , Ac3(Acm) = 784 , Ar3(Arcm) = 685 , Ar1 = 640 , Mn = 175 |
Weldability: | is not used. |
Flakes : | predisposed |
Temper brittleness: | predisposed |
T | E 10- 5 | a 10 6 | l | r | C | R 10 9 |
Grade | MPa | 1/Grade | Watt/(m·Grade) | kg/m3 | J/(kg·Grade) | Ohm·m |
20 | 7840 | |||||
100 | 37 | 440 | ||||
200 | 34 | 460 | ||||
300 | 32 | 500 | ||||
400 | 32 | 570 | ||||
500 | 32 | 680 | ||||
600 | 30 | 800 | ||||
700 | 23 | 940 | ||||
800 | 20 | 1100 | ||||
900 | 14 | 500 | ||||
1000 | 500 | |||||
T | E 10- 5 | a 10 6 | l | r | C | R 10 9 |
Mechanical properties : | |
sв | - Tensile strength , [MPa] |
sT | - Yield stress, [MPa] |
d5 | - Specific elongation at fracture , [ % ] |
y | - Reduction of area , [ % ] |
KCU | - Impact strength , [ kJ / m2] |
HB | - Brinell hardness , [MPa] |
Physical properties : | |
T | - Test temperature , [Grade] |
E | - Young modulus , [MPa] |
a | - Coefficient of linear expansion (range 20o - T ) , [1/Grade] |
l | - Termal (heat) condition coefficient , [Watt/(m·Grade)] |
r | - Density , [kg/m3] |
C | - Specific heat ( range 20o - T ), [J/(kg·Grade)] |
R | - Electrical resistance , [Ohm·m] |
Weldability : | |
without limitations | - welding is done without heating and subsequent heat treeting |
limited weldability | - welding is possible under heating up to 100-120 grade and subsequent heat treeting |
hard weldability | - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing |
© 2003 - 2024 Database of Steel and Alloy (russian title is the Marochnik)
Administration of the Marochnik is not responsible for the content's use. |