Grade : | 45KHNM ( 45ХНМ ) |
Substitute: | 40ХН2МА |
Classification : | Tool steel for roller |
Equivalent grades: | Is absent |
C | Si | Mn | Ni | S | P | Cr | Mo |
0.4 - 0.5 | 0.17 - 0.37 | 0.5 - 0.8 | 1.2 - 1.6 | max 0.04 | max 0.04 | 1.3 - 1.7 | 0.1 - 0.3 |
Ac1 = 750 , Ac3(Acm) = 780 |
Assortment | Dimension | Direct. | sв | sT | d5 | y | KCU | Heat treatment |
- | mm | - | MPa | MPa | % | % | kJ / m2 | - |
Forging | 100 - 300 | 635 | 440 | 14 | 40 | 540 | Normalizing |
Brinell hardness for 45KHNM ( 45ХНМ ) (normalize) , | HB 10 -1 = 197 - 248 MPa |
Brinell hardness for 45KHNM ( 45ХНМ ) (quenching, tempering) , | HB 10 -1 = 197 - 262 MPa |
Weldability: | is not used. |
Flakes : | predisposed |
Temper brittleness: | weakly predisposed |
B03 - Metal forming treatment. Forgings |
Mechanical properties : | |
sв | - Tensile strength , [MPa] |
sT | - Yield stress, [MPa] |
d5 | - Specific elongation at fracture , [ % ] |
y | - Reduction of area , [ % ] |
KCU | - Impact strength , [ kJ / m2] |
HB | - Brinell hardness , [MPa] |
Physical properties : | |
T | - Test temperature , [Grade] |
E | - Young modulus , [MPa] |
a | - Coefficient of linear expansion (range 20o - T ) , [1/Grade] |
l | - Termal (heat) condition coefficient , [Watt/(m·Grade)] |
r | - Density , [kg/m3] |
C | - Specific heat ( range 20o - T ), [J/(kg·Grade)] |
R | - Electrical resistance , [Ohm·m] |
Weldability : | |
without limitations | - welding is done without heating and subsequent heat treeting |
limited weldability | - welding is possible under heating up to 100-120 grade and subsequent heat treeting |
hard weldability | - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing |