Database of Steel and Alloy (Marochnik) |
Home | Steel and Alloy | Search | Equivalent Grades | GOST Standards | Grading | Contacts |
Grade : | 08KH18T1 ( 08Х18Т1 ) ( 0Х18Т1 ) |
Classification : | Corrosion-resistant high-temperature steel |
Equivalent grades: | Is absent |
C | Si | Mn | Ni | S | P | Cr | Ti | Cu |
max 0.08 | max 0.8 | max 0.7 | max 0.6 | max 0.025 | max 0.035 | 17 - 19 | 0.6 - 1 | max 0.3 |
Assortment | Dimension | Direct. | sв | sT | d5 | y | KCU | Heat treatment |
- | mm | - | MPa | MPa | % | % | kJ / m2 | - |
Sheet, GOST 5582-75 | to 4 | dihedral | 460 | 30 | Annealing 830 - 860oC, air, | |||
Pipe, GOST 11068-81 | 450 | 28 |
Weldability: | limited weldability. |
T | E 10- 5 | a 10 6 | l | r | C | R 10 9 |
Grade | MPa | 1/Grade | Watt/(m·Grade) | kg/m3 | J/(kg·Grade) | Ohm·m |
20 | 7720 |
B23 - Sheets and Strips |
B33 - Sheets and Strips |
В62 - Steel pipes and connecting parts to them |
Mechanical properties : | |
sв | - Tensile strength , [MPa] |
sT | - Yield stress, [MPa] |
d5 | - Specific elongation at fracture , [ % ] |
y | - Reduction of area , [ % ] |
KCU | - Impact strength , [ kJ / m2] |
HB | - Brinell hardness , [MPa] |
Physical properties : | |
T | - Test temperature , [Grade] |
E | - Young modulus , [MPa] |
a | - Coefficient of linear expansion (range 20o - T ) , [1/Grade] |
l | - Termal (heat) condition coefficient , [Watt/(m·Grade)] |
r | - Density , [kg/m3] |
C | - Specific heat ( range 20o - T ), [J/(kg·Grade)] |
R | - Electrical resistance , [Ohm·m] |
Weldability : | |
without limitations | - welding is done without heating and subsequent heat treeting |
limited weldability | - welding is possible under heating up to 100-120 grade and subsequent heat treeting |
hard weldability | - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing |
© 2003 - 2025 Database of Steel and Alloy (russian title is the Marochnik)