Chemical composition in % for grade   18G2АF   ( 18Г2АФ )
C Si Mn Ni S P Cr V N Cu As
0.14 - 0.22max   0.171.3 - 1.7max   0.3max   0.035max   0.03max   0.30.08 - 0.150.015 - 0.03max   0.3max   0.08


Mechanical properties under Т=20oС for grade   18G2АF   ( 18Г2АФ )
Assortment Dimension Direct. sв sT d5 y KCU Heat treatment
- mm - MPa MPa % % kJ / m2 -
Sheet     600 450 19    


Technological properties for grade   18G2АF   ( 18Г2АФ )
  Weldability: without limitations.


Equivalent steels for grade     18G2АF   ( 18Г2АФ )
Warning! Indicated both exact and nearest equivalents.
USAGermanyJapanFranceEnglandEuropeanItalySpainChinaSwedenHungaryPolandCzechiaSwitzerland
-DIN,WNrJIS AFNORBSEN UNIUNEGBSSMSZPNCSNSNV
A350(LF6CL1)
A350(LF6CL2)
A350(LF6CL3)
K02900
K12202
22MnV6
P355N
P460N
SM520B
SM520C
P460N
55F
P460N
P460N
P460NH
S460N
FeE460KG
P460N
AE460KG
P460N
15MnVNR
18MnMoNbR
Q460C
2143
E460D
18G2AV
19G2FA
13220
StE47

Types of delivery of grade   18G2АF   ( 18Г2АФ )
В22 - Graded and shaped rolling
B23 - Sheets and Strips
В62 - Steel pipes and connecting parts to them


Specification :
Mechanical properties :
sв - Tensile strength , [MPa]
sT - Yield stress, [MPa]
d5 - Specific elongation at fracture , [ % ]
y - Reduction of area , [ % ]
KCU - Impact strength , [ kJ / m2]
HB - Brinell hardness , [MPa]

Physical properties :
T - Test temperature , [Grade]
E - Young modulus , [MPa]
a - Coefficient of linear expansion (range 20o - T ) , [1/Grade]
l - Termal (heat) condition coefficient , [Watt/(m·Grade)]
r - Density , [kg/m3]
C - Specific heat ( range 20o - T ), [J/(kg·Grade)]
R - Electrical resistance , [Ohm·m]

Weldability :
without limitations - welding is done without heating and subsequent heat treeting
limited weldability - welding is possible under heating up to 100-120 grade and subsequent heat treeting
hard weldability - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing

  18G2АF   ( 18Г2АФ ) - Structural steel for welding construct: chemical composition, mechanical and physical properties, hardness
Database of steels and alloys (Marochnik) contains information about chemical composition and properties more then 3000 steels and alloys

    ©   2003 - 2019         Database of Steel and Alloy (russian title is the Marochnik)
Administration of the Marochnik is not responsible for the content's use.
Previous address of this website was splav.kharkov.com
Рейтинг@Mail.ru