Database of Steel and Alloy (Marochnik)

  Home     Steel and Alloy     Search     Equivalent Grades     GOST Standards     Grading     Contacts  
    YOU HERE:   Steel and Alloy   ->   High-temperature or heat-resistant steel and alloy

Characteristics for grade     08KH16N11M3   ( 08Х16Н11М3 )

      Grade :     08KH16N11M3   ( 08Х16Н11М3 )
      Classification :   High alloy high-temperature steel
      Equivalent grades:   Go here



Chemical composition in % for grade   08KH16N11M3   ( 08Х16Н11М3 )
C Si Mn Ni S P Cr Mo
max   0.08max   0.61 - 1.58.5 - 10max   0.02max   0.03515.5 - 171.5 - 2


Mechanical properties under Т=20oС for grade   08KH16N11M3   ( 08Х16Н11М3 )
Assortment Dimension Direct. sв sT d5 y KCU Heat treatment
- mm - MPa MPa % % kJ / m2 -
Pipe   longitudinal 540 220 40 551500 
Pipe   dihedral 540 220 35 501400 


Technological properties for grade   08KH16N11M3   ( 08Х16Н11М3 )
  Weldability: without limitations.


Physical properties for grade   08KH16N11M3   ( 08Х16Н11М3 )
T E 10- 5 a 10 6 l r C R 10 9
Grade MPa 1/Grade Watt/(m·Grade) kg/m3 J/(kg·Grade) Ohm·m
20 2.14     7900    
100   17.1        
200   17.6        
300   18.1        
400 1.84 18.4        
500 1.75 19        
600   19.3        
700   19.6        
800   19.8        
T E 10- 5 a 10 6 l r C R 10 9


Equivalent steels for grade     08KH16N11M3   ( 08Х16Н11М3 )
Warning! Indicated both exact and nearest equivalents.
USAGermanyJapanEuropeanChinaSwedenPolandCzechia
-DIN,WNrJIS EN GBSSPNCSN
316
X5CrNiMo17-12-2
SUS316
1.4401
X5CrNiMo17-12-2
0Cr17Ni12Mo2
2347
0H17N12M2T
17346


Specification :
Mechanical properties :
sв - Tensile strength , [MPa]
sT - Yield stress, [MPa]
d5 - Specific elongation at fracture , [ % ]
y - Reduction of area , [ % ]
KCU - Impact strength , [ kJ / m2]
HB - Brinell hardness , [MPa]

Physical properties :
T - Test temperature , [Grade]
E - Young modulus , [MPa]
a - Coefficient of linear expansion (range 20o - T ) , [1/Grade]
l - Termal (heat) condition coefficient , [Watt/(m·Grade)]
r - Density , [kg/m3]
C - Specific heat ( range 20o - T ), [J/(kg·Grade)]
R - Electrical resistance , [Ohm·m]

Weldability :
without limitations - welding is done without heating and subsequent heat treeting
limited weldability - welding is possible under heating up to 100-120 grade and subsequent heat treeting
hard weldability - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing

  08KH16N11M3   ( 08Х16Н11М3 ) - High alloy high-temperature steel: chemical composition, mechanical and physical properties, hardness
Database of steels and alloys (Marochnik) contains information about chemical composition and properties more then 3000 steels and alloys

    ©   2003 - 2018         Database of Steel and Alloy (russian title is the Marochnik)
Administration of the Marochnik is not responsible for the content's use.
Previous address of this website was splav.kharkov.com
Рейтинг@Mail.ru