Database of Steel and Alloy (Marochnik) |
Home | Steel and Alloy | Search | Equivalent Grades | GOST Standards | Grading | Contacts |
Grade : | R6M5 ( Р6М5 ) |
Classification : | High speed tool steel |
Equivalent grades: | Go here |
C | Si | Mn | Ni | S | P | Cr | Mo | W | V | Co | Cu |
0.82 - 0.9 | 0.2 - 0.5 | 0.2 - 0.5 | max 0.6 | max 0.025 | max 0.03 | 3.8 - 4.4 | 4.8 - 5.3 | 5.5 - 6.5 | 1.7 - 2.1 | max 0.5 | max 0.25 |
Ac1 = 815 , Ar1 = 730 |
Brinell hardness for R6M5 ( Р6М5 ) (annealing) , GOST 19265-73 | HB 10 -1 = 255 MPa |
USA | Germany | Japan | France | England | European | Italy | Spain | China | Sweden | Bulgaria | Hungary | Poland | Romania | Czechia | Austria | South Korea | |||||||||||||||||||||||||||||||||||
- | DIN,WNr | JIS | AFNOR | BS | EN | UNI | UNE | GB | SS | BDS | MSZ | PN | STAS | CSN | ONORM | KS | |||||||||||||||||||||||||||||||||||
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
В22 - Graded and shaped rolling |
В32 - Graded and shaped rolling |
B33 - Sheets and Strips |
Mechanical properties : | |
sв | - Tensile strength , [MPa] |
sT | - Yield stress, [MPa] |
d5 | - Specific elongation at fracture , [ % ] |
y | - Reduction of area , [ % ] |
KCU | - Impact strength , [ kJ / m2] |
HB | - Brinell hardness , [MPa] |
Physical properties : | |
T | - Test temperature , [Grade] |
E | - Young modulus , [MPa] |
a | - Coefficient of linear expansion (range 20o - T ) , [1/Grade] |
l | - Termal (heat) condition coefficient , [Watt/(m·Grade)] |
r | - Density , [kg/m3] |
C | - Specific heat ( range 20o - T ), [J/(kg·Grade)] |
R | - Electrical resistance , [Ohm·m] |