Grade : | 30GL ( 30ГЛ ) |
Classification : | Casting alloy steel for general purposes |
Equivalent grades: | Is absent |
C | Si | Mn | S | P |
0.25 - 0.32 | 0.2 - 0.5 | 1.4 - 1.7 | max 0.04 | max 0.04 |
Assortment | Dimension | Direct. | sв | sT | d5 | y | KCU | Heat treatment |
- | mm | - | MPa | MPa | % | % | kJ / m2 | - |
Casting, GOST 977-88 | 579 | 334 | 20 | 25 | 206 | Normalizing | ||
Casting, GOST 977-88 | 628 | 481 | 16 | 20 | 235 | Guenching and drawing | ||
Casting, GOST 21357-87 | 660 | 490 | 10 | 20 | Guenching 920 - 950oC, water, Drawing 600 - 650oC, |
Normalizing 860 - 890 ° C, Tempering 550 - 650 ° C |
Hardening 840 - 860 ° C, Tempering 570 - 610 ° C |
B82 - Steel Castings |
B83 - Castings with special properties (cast iron and steel) |
Mechanical properties : | |
sв | - Tensile strength , [MPa] |
sT | - Yield stress, [MPa] |
d5 | - Specific elongation at fracture , [ % ] |
y | - Reduction of area , [ % ] |
KCU | - Impact strength , [ kJ / m2] |
HB | - Brinell hardness , [MPa] |
Physical properties : | |
T | - Test temperature , [Grade] |
E | - Young modulus , [MPa] |
a | - Coefficient of linear expansion (range 20o - T ) , [1/Grade] |
l | - Termal (heat) condition coefficient , [Watt/(m·Grade)] |
r | - Density , [kg/m3] |
C | - Specific heat ( range 20o - T ), [J/(kg·Grade)] |
R | - Electrical resistance , [Ohm·m] |
© 2003 - 2025 Database of Steel and Alloy (russian title is the Marochnik)
Administration of the Marochnik is not responsible for the content's use. |