Database of Steel and Alloy (Marochnik) |
Home | Steel and Alloy | Search | Equivalent Grades | GOST Standards | Grading | Contacts |
Grade : | 5KH3V3MFS ( 5Х3В3МФС ) ( ДИ23 ) |
Classification : | Die tool steel |
Equivalent grades: | Go here |
C | Si | Mn | Ni | S | P | Cr | Mo | W | V | Nb | Cu |
0.45 - 0.52 | 0.5 - 0.8 | 0.2 - 0.5 | max 0.4 | max 0.03 | max 0.03 | 2.5 - 3.2 | 0.8 - 1.1 | 3 - 3.6 | 1.5 - 1.8 | 0.05 - 0.15 | max 0.3 |
Ac1 = 780 , Ac3(Acm) = 920 , Ar3(Arcm) = 725 |
Assortment | Dimension | Direct. | sв | sT | d5 | y | KCU | Heat treatment |
- | mm | - | MPa | MPa | % | % | kJ / m2 | - |
Bars | 15 | 1680 | 1500 | 8 | 38 | 250 | Guenching 1130oC, oil, Drawing |
Brinell hardness for 5KH3V3MFS ( 5Х3В3МФС ) (annealing) , GOST 5950-2000 | HB 10 -1 = 229 - 241 MPa |
Germany | |||
DIN,WNr | |||
|
В32 - Graded and shaped rolling |
Mechanical properties : | |
sв | - Tensile strength , [MPa] |
sT | - Yield stress, [MPa] |
d5 | - Specific elongation at fracture , [ % ] |
y | - Reduction of area , [ % ] |
KCU | - Impact strength , [ kJ / m2] |
HB | - Brinell hardness , [MPa] |
Physical properties : | |
T | - Test temperature , [Grade] |
E | - Young modulus , [MPa] |
a | - Coefficient of linear expansion (range 20o - T ) , [1/Grade] |
l | - Termal (heat) condition coefficient , [Watt/(m·Grade)] |
r | - Density , [kg/m3] |
C | - Specific heat ( range 20o - T ), [J/(kg·Grade)] |
R | - Electrical resistance , [Ohm·m] |