Grade : | 08KH18N12B ( 08Х18Н12Б ) ( 0Х18Н12Б ЭИ402 ) |
Classification : | Corrosion-resistant steel for general purposes |
Equivalent grades: | Go here |
C | Si | Mn | Ni | S | P | Cr | - |
max 0.08 | max 0.8 | max 2 | 11 - 13 | max 0.02 | max 0.035 | 17 - 19 | 10*С-1.1 ниобий |
Assortment | Dimension | Direct. | sв | sT | d5 | y | KCU | Heat treatment |
- | mm | - | MPa | MPa | % | % | kJ / m2 | - |
Pipe cooling strain, GOST 9941-81 | 529 | 37 | ||||||
Pipe hot strain, GOST 9940-81 | 510 | 38 | ||||||
Bar, GOST 5949-75 | to Ø 60 | 490 | 175 | 40 | 55 | Guenching 1050 - 1100oC, air, | ||
Sheet trick, GOST 7350-77 | 510 | 205 | 40 | Guenching 1000 - 1100oC,Cooling air, | ||||
Sheet thin, GOST 5582-75 | 530 | 40 | Guenching 1050 - 1080oC, air, |
T | E 10- 5 | a 10 6 | l | r | C | R 10 9 |
Grade | MPa | 1/Grade | Watt/(m·Grade) | kg/m3 | J/(kg·Grade) | Ohm·m |
20 | 2.02 | 7900 | 730 | |||
100 | 15.9 |
USA | Germany | Japan | France | England | European | Italy | Spain | China | Sweden | ||||||||||||||||||||
- | DIN,WNr | JIS | AFNOR | BS | EN | UNI | UNE | GB | SS | ||||||||||||||||||||
|
|
|
|
|
|
|
|
|
|
В22 - Graded and shaped rolling |
B23 - Sheets and Strips |
В32 - Graded and shaped rolling |
B33 - Sheets and Strips |
В62 - Steel pipes and connecting parts to them |
Mechanical properties : | |
sв | - Tensile strength , [MPa] |
sT | - Yield stress, [MPa] |
d5 | - Specific elongation at fracture , [ % ] |
y | - Reduction of area , [ % ] |
KCU | - Impact strength , [ kJ / m2] |
HB | - Brinell hardness , [MPa] |
Physical properties : | |
T | - Test temperature , [Grade] |
E | - Young modulus , [MPa] |
a | - Coefficient of linear expansion (range 20o - T ) , [1/Grade] |
l | - Termal (heat) condition coefficient , [Watt/(m·Grade)] |
r | - Density , [kg/m3] |
C | - Specific heat ( range 20o - T ), [J/(kg·Grade)] |
R | - Electrical resistance , [Ohm·m] |
© 2003 - 2025 Database of Steel and Alloy (russian title is the Marochnik)