Characteristics for grade     S285   ( С285 )



      Grade :     S285   ( С285 )
      Substitute:   Ст3сп, Ст3Гпс, Ст3Гсп
      Classification :   Steel for structural constructions
      Equivalent grades:   Go here



Chemical composition in % for grade   S285   ( С285 )
C Si Mn Ni S P Cr N Cu
max   0.220.15 - 0.3max   0.65max   0.3max   0.05max   0.04max   0.3max   0.012max   0.3


Mechanical properties under Т=20oС for grade   S285   ( С285 )
Assortment Dimension Direct. sв sT d5 y KCU Heat treatment
- mm - MPa MPa % % kJ / m2 -
Sheet, GOST 27772-88 2 - 3.9   390 285 17    
Sheet, GOST 27772-88 4 - 10   390 275 24    
Sheet, GOST 27772-88 10 - 20   380 265 23    


Technological properties for grade   S285   ( С285 )
  Weldability: without limitations.


Equivalent steels for grade     S285   ( С285 )
Warning! Indicated both exact and nearest equivalents.
USAGermanyJapanFranceEnglandEuropeanItalyChinaSwedenPolandCzechiaAustria
-DIN,WNrJIS AFNORBSEN UNIGBSSPNCSNONORM
Gr.50
1.0050
St50-2
SS490
A50
43/35HS
1.0050
E295
Fe490
Q275
2172
St5
11500
St50F



Types of delivery of grade   S285   ( С285 )
В22 - Graded and shaped rolling
B23 - Sheets and Strips


Specification :
Mechanical properties :
sв - Tensile strength , [MPa]
sT - Yield stress, [MPa]
d5 - Specific elongation at fracture , [ % ]
y - Reduction of area , [ % ]
KCU - Impact strength , [ kJ / m2]
HB - Brinell hardness , [MPa]

Physical properties :
T - Test temperature , [Grade]
E - Young modulus , [MPa]
a - Coefficient of linear expansion (range 20o - T ) , [1/Grade]
l - Termal (heat) condition coefficient , [Watt/(m·Grade)]
r - Density , [kg/m3]
C - Specific heat ( range 20o - T ), [J/(kg·Grade)]
R - Electrical resistance , [Ohm·m]

Weldability :
without limitations - welding is done without heating and subsequent heat treeting
limited weldability - welding is possible under heating up to 100-120 grade and subsequent heat treeting
hard weldability - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing

  S285   ( С285 ) - Steel for structural constructions: chemical composition, mechanical and physical properties, hardness
Database of steels and alloys (Marochnik) contains information about chemical composition and properties more then 3000 steels and alloys

    ©   2003 - 2025         Database of Steel and Alloy (russian title is the Marochnik)
Administration of the Marochnik is not responsible for the content's use.
Рейтинг@Mail.ru