Characteristics for grade     St0   ( Ст0 )

      Grade :     St0   ( Ст0 )
      Classification :   Normal quality structural carbon steel
      Equivalent grades:   Go here



Chemical composition in % for grade   St0   ( Ст0 )
C S P
max   0.23max   0.06max   0.07


Mechanical properties under Т=20oС for grade   St0   ( Ст0 )
Assortment Dimension Direct. sв sT d5 y KCU Heat treatment
- mm - MPa MPa % % kJ / m2 -
Rolled stock, GOST 535-2005     300   15-18   
Sheet trick, GOST 14637-89     300   20-23   
Wire rods , GOST 30136-95     420-470    58-68  


Technological properties for grade   St0   ( Ст0 )
  Weldability: without limitations.
 Flakes : not predisposed
Temper brittleness: not predisposed


Physical properties for grade   St0   ( Ст0 )
T E 10- 5 a 10 6 l r C R 10 9
Grade MPa 1/Grade Watt/(m·Grade) kg/m3 J/(kg·Grade) Ohm·m
20       7850    


Equivalent steels for grade     St0   ( Ст0 )
Warning! Indicated both exact and nearest equivalents.
USAGermanyJapanFranceEnglandEuropeanItalyBelgiumSpainChinaSwedenBulgariaHungaryPolandRomaniaCzechiaAustriaInter
-DIN,WNrJIS AFNORBSEN UNINBNUNEGBSSBDSMSZPNSTASCSNONORMISO
A283(A)
A366
Gr.A
1.0035
1.0035
Fe310-0
S185
St33
St33-1
St33-2
SS330
A33
S185
15HR
15HS
Fe310-0
HR15
S185
1.0035
S185
Fe320
S185
FE310-0
A310-0
S185
Q195
Q195-b
Q195-F
Q195-Z
1300
ASt0
S185
Fe310O
S185
St0S
OL32.1
10000
10004
St00H
E185
Fe310

Types of delivery of grade   St0   ( Ст0 )
В20 - Classification, nomenclature and general norms
В22 - Graded and shaped rolling
B23 - Sheets and Strips
B24 - Ribbons
B34 - Ribbons
В62 - Steel pipes and connecting parts to them
В71 - Low-carbon steel wire
В72 - Medium-high and high-carbon steel wire


Specification :
Mechanical properties :
sв - Tensile strength , [MPa]
sT - Yield stress, [MPa]
d5 - Specific elongation at fracture , [ % ]
y - Reduction of area , [ % ]
KCU - Impact strength , [ kJ / m2]
HB - Brinell hardness , [MPa]

Physical properties :
T - Test temperature , [Grade]
E - Young modulus , [MPa]
a - Coefficient of linear expansion (range 20o - T ) , [1/Grade]
l - Termal (heat) condition coefficient , [Watt/(m·Grade)]
r - Density , [kg/m3]
C - Specific heat ( range 20o - T ), [J/(kg·Grade)]
R - Electrical resistance , [Ohm·m]

Weldability :
without limitations - welding is done without heating and subsequent heat treeting
limited weldability - welding is possible under heating up to 100-120 grade and subsequent heat treeting
hard weldability - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing

  St0   ( Ст0 ) - Normal quality structural carbon steel: chemical composition, mechanical and physical properties, hardness
Database of steels and alloys (Marochnik) contains information about chemical composition and properties more then 3000 steels and alloys

    ©   2003 - 2019         Database of Steel and Alloy (russian title is the Marochnik)
Administration of the Marochnik is not responsible for the content's use.
Previous address of this website was splav.kharkov.com
Рейтинг@Mail.ru